在 IF 钢的生产过程中,退火是非常关键的工艺环节。针对酒钢 CSP 生产的 Ti-IF 钢进行研究,分析了在罩式退火工艺条件下,罩式退火工艺对 Ti-IF 钢组织与性能的影响。结果表明:退火温度从680℃上升到750℃保温2 h,试样抗拉强度从284下降到268 MPa,屈服强度从114下降到96 MPa,屈强比从0.40降低到0.36,伸长率从44.3%提高到47%,塑性应变比 r 90值从2.22升高到2.60。

Annealing is the key limit in the productive process of IF steel.Focusing on the TI-IF steel produced by CSP process in JiuSteel,the effect of batch type annealing process on microstructure and properties of Ti-IF steel is investigated.The results indicate that when the annealing temperature increases from 680 ℃ to 750 ℃ within 2 h, tensile strength reduces from 284 to 268 MPa,yield strength reduces from 114 MPa to 96 MPa ,yield ratio decrea-ses from 0.40 to 0.36,elongation increases from 44.25% to 47% and r 90 increases from 2.22 to 2.60.

参考文献

[1] 康永林.现代汽车板的质量控制与成形性[M].北京:冶金工业出版社,1999.,1999.
[2] 潘秀兰,王艳红,梁慧智,冯士超.国内外超低碳IF钢炼钢工艺分析[J].鞍钢技术,2009(01):6-9.
[3] Akbari G H,Sellars C M,Whiteman J A .Mierostrueture de-velopment during warm rolling of an IF steel[J].Actamateri-alia,1997,45(12):50.,1997.
[4] 高攀,田志红,崔阳,胡帅,李永林,朱立新.IF钢非稳态浇铸铸坯洁净度分析[J].钢铁,2012(07):31-35.
[5] 徐海卫,于洋,李飞,朱国森,李本海.IF钢热轧薄板边部翘皮缺陷的产生原因及机制[J].钢铁,2012(09):53-56.
[6] 侯自勇,许云波,吴迪,王国栋.一种高Nb-IF冷轧薄板钢的组织性能及织构[J].钢铁研究学报,2012(05):47-52,62.
[7] 水恒勇,赵爱民,汪志刚,王纯,苏岚.再结晶退火温度对高强IF钢组织性能及织构的影响[J].轧钢,2012(02):8-11.
[8] 穆海玲,李清燕,裴新华,赵骧.热轧和卷取温度对IF钢织构的影响[J].轧钢,2012(03):17-19.
[9] 王昭东,郭艳辉,赵忠,孙大庆.应用铁素体区热轧工艺开发超低碳热轧深冲板[J].东北大学学报(自然科学版),2005(08):747-750.
[10] 刘战英,周满春,王涛,刘相华,王国栋.IF钢铁素体区热轧工艺参数对深冲性能的影响[J].钢铁研究学报,2007(04):44-46,94.