对低层错能Fe-26Mn-6Si-7Cr-1Cu形状记忆合金和0Cr13Ni5Mo不锈钢进行了空蚀试验.结果表明,Fe-26Mn-6Si-7Cr-1Cu形状记忆合金抗空蚀性能优于0Crl3Ni5Mo不锈钢.空蚀过程中应变诱发马氏体转变是该形状记忆合金具有良好抗空蚀性能的主要原因.

参考文献

[1] D. Y. Li .A new type of wear-resistant material: pseudo-elastic TiNi alloy[J].Wear: an International Journal on the Science and Technology of Friction, Lubrication and Wear,1998(2):116-123.
[2] Richman R H;Rao A S;Kung D .Cavitation erosion of NiTi explosively welded to steel[J].Wear,1995,181-183:80-85.
[3] Richman R H;Hodgson D E;Rao A S .Cavitation erosion of two NiTi alloys[J].Wear,1992,157:401-407.
[4] Wu S K;Lin H C;Yeh C H .A comparision of the cavitation erosion resistance of TiNi alloys SUS304 stainless steel and Ni-based self-fluxing alloy[J].Wear,2000,244:85-93.
[5] Olson G B;Cohen M .A general mechanism of martensitic nucleation: Part 1. General concepts and the fcc-hcp transformation[J].Metallurgical and Materials Transactions A:Physical Metallurgy and Materials Science,1976,7:1897-1904.
[6] Olson G B;Cohen M .A general mechanism of martensitic nucleation: Part Ⅲ Kinetics of martensitic nucleation[J].Metallurgical and Materials Transactions A:Physical Metallurgy and Materials Science,1976,7:1915-1923.