研究了用化学还原法从电镀银废液中回收银时,Na_2S_2O_4/Ag~+摩尔比、温度等因素对银回收率的影响,得到的最佳回收工艺条件为:Na_2S_2O_4 /Ag~+摩尔比为2.5,温度35℃,pH = 7.5,搅拌速度300 r/min,用此工艺银的回收率可达99.98%.采用XRD、XRF、TEM、SAED对回收的银粉体进行了表征,银粉纯度较高,成球链状分布,平均粒径为175.8 nm.
In this paper, silver was recovered from the silver electrolytic effluents by chemical reduction method. The effects of various factors such as Na_2S_2O_4/Ag~+ ratio, temperature on the silver recovery rate were systematically studied. The optimum technical condition was obtained as follows: Na_2S_2O_4/Ag~+ =2.5, 35℃, pH 7.5 with a stirring speed 300 r/min. With this technical process, the silver recovery rate can reach to 99.98%. The recovered silver powders were characterized by X-ray diffraction (XRD), X-ray fluorescence (XRF), transmission electron microscopy (TEM) and the corresponding selected area electron diffraction (SAED). They are chain-spherical with mean diameters of 175.8 nm and high purity.
参考文献
[1] | 石和清.银价:向上空间渐开新高仍将可期-2008年1-2月白银市场述评及后市展望[J].中国金属通报,2008(11):8-12. |
[2] | 蔡积庆.电镀银和银合金[J].电镀与环保,2002(03):8-10. |
[3] | 张顺利.电镀废水处理技术概况与展望[J].科技信息(科学·教研),2007(21):28. |
[4] | 夏士朋.利用硼氢化钠从含银废液中回收银[J].化学世界,1994(07):379-380. |
[5] | I. Rivera;F. Patino;M. Cruells .Precipitacion de plata de efluentes electroliticos[J].Revista de Metalurgia,2004(5):369-373. |
[6] | I. Rivera;A. Roca;M. Cruells .Study of silver precipitation in thiosulfate solutions using sodium dithionite. Application to an industrial effluent[J].Hydrometallurgy,2007(1/2):89-98. |
[7] | GB 11908-1989.GB 11908-1989.水质银的测定镉试剂2B分光光度法[S].北京:中国标准出版社,1989. |
[8] | 段志伟,张振忠,江成军,王超.直流电弧等离子体法制备超细Ag粉研究[J].铸造技术,2007(01):23-26. |
- 下载量()
- 访问量()
- 您的评分:
-
10%
-
20%
-
30%
-
40%
-
50%