对高牌号无取向电工钢35W300的成品进行了第二次退火,对第二次退火后的成品性能、纵横向磁性能差异和组织变化进行了分析.结果表明,随着第二次退火温度的升高,晶粒长大,磁性能优化.铁损平均值下降0.087 5 W/kg,磁感平均值升高0.008 T.第二次退火温度为820℃的产品的磁性能能够满足用户使用要求.

参考文献

[1] Yuriy Sidor;Frantisek Kovac .Microstructural aspects of grain growth kinetics in non-oriented electrical steels[J].Materials Characterization,2005(1):1-11.
[2] A. Chaudhury;R. Khatirkar;N.N. Viswanathan;V. Singal;A. Ingle;S. Joshi;I. Samajdar .Low silicon non-grain-oriented electrical steel: Linking magnetic properties with metallurgical factors[J].Journal of Magnetism and Magnetic Materials,2007(1):21-28.
[3] C.M.B. Bacaltchuk;G.A. Castello-Branco;M. Ebrahimi .Effect of magnetic field applied during secondary annealing on texture and grain size of silicon steel[J].Scripta materialia,2003(9):1343-1347.
[4] Park, JT;Szpunar, JA .Effect of initial grain size on texture evolution and magnetic properties in nonoriented electrical steels[J].Journal of Magnetism and Magnetic Materials,2009(13):1928-1932.
[5] 高振宇,罗理,李文权,朱丽君,王舒宏.高牌号无取向电工钢技术发展及应用[J].鞍钢技术,2011(02):6-10,24.
[6] 赵亚慧,朱国辉,王立涛,高海建.退火温度对CSP生产薄规格无取向电工钢性能的影响[J].金属功能材料,2012(02):18-22.
[7] 项利,刘昀,张晨,裴英豪,王立涛,仇圣桃.常化对含硅1.6%的无取向电工钢组织和织构的影响[J].钢铁研究学报,2012(11):34-38.
[8] 赵国君.关于卷铁心消除内应力退火问题的探讨[J].变压器,2004(02):22-24.
[9] 熊火,召行,黄官平.用井式退火炉对卷铁心退火[J].变压器,2001(06):9-10.
[10] 张付军,彭魁先,王克太.浅谈卷铁心变压器铁心退火要点[J].变压器,2002(12):27-28.
上一张 下一张
上一张 下一张
计量
  • 下载量()
  • 访问量()
文章评分
  • 您的评分:
  • 1
    0%
  • 2
    0%
  • 3
    0%
  • 4
    0%
  • 5
    0%