对橡胶等静压成型(Rubber isostatic pressing,RIP)制备纳米Y-TZP陶瓷作了初步研究.研究结果表明,通过RIP成型,可以获得相对密度较高、体积较大的ZrO2(3Y)素坯,并在较低温度下无压烧结得到纳米Y-TZP陶瓷.在1100℃下烧结2h所得的Y-TZP陶瓷的相对密度可达97%,晶粒仅为70nm左右.相对密度较高、平均孔径小是RIP成型素坯烧结温度低的主要原因.

A new forming method called RIP was applied to fabricate Y-TZP nano ceramics. With RIP, a high pressure of about 1GPa was attained; a green compact
with a weight of about 16g and a relative density of about 56% wasobtained. Y-TZP nano-ceramics having a grain size of about 70nm were
obtained when sintered at 1100℃ for 2h. The results show that the sintering ability of the green compact is so good that it can be sintered to 97% at a low
temperature of 1100℃. The relative high density of the green compact and the small pore size are the main reasons for the excellent
sintering ability.

参考文献

[1] Srdi\acute{c V V, Minterer M, Hahn H. J. Am. Ceram. Soc., 2000, 83 (4): 729--736.
[2] Yan D S, Qiu H B, Zheng Y S, et al. Nanostructured Materials, 1997, 9 (1-8): 441--450.
[3] Mayo M J. International Materials Reviews, 1996, 41 (3): 93--115.
[4] Ivanov V, Kotov Y A, Samatov O H, et al. Nanostructured Materials, 1995, 6 (1-4): 287--290.
[5] 高濂, 李蔚, 王宏志, 等(GAO Lian, et al). 无机材料学报(Journal of Inorganic Materials), 2000, 15 (6): 1005--1998.
[6] Gao L, Li W, Wang H Z, et al. J. Euro. Ceram. Soc., 2001, 21 (2): 135--138.
[7] Introduction of RUBBER ISOSTATIC PRESSING. Intermetallics Co., L td. 2-4.
[8] Chen D J, Mayo M J. NanoStructured Materials, 1993, 2 (5): 609--613.
上一张 下一张
上一张 下一张
计量
  • 下载量()
  • 访问量()
文章评分
  • 您的评分:
  • 1
    0%
  • 2
    0%
  • 3
    0%
  • 4
    0%
  • 5
    0%