欢迎登录材料期刊网

材料期刊网

高级检索

以受阻胺光稳定剂和紫外线吸收剂对聚甲醛( POM)进行光稳定化耐候改性,并对制得的耐候POM的力学性能和人工加速老化行为进行了测试和评价。结果表明,经氙灯人工加速老化1000 h后,试样的拉伸强度保持率、断裂伸长率保持率和缺口冲击强度保持率分别达到103%、76.2%和84.4%,色差由7.6减小至0.8,远优于未经光稳定化处理的POM的相应性能。

Weathering polyoxymethylene ( POM) materials modified with compounded hindered amine light stabi-lizers and ultraviolet absorbers were prepared ,and their mechanical properties and artificial accelerated aging behav -iors were tested and evaluated.It has been found that the retention of tensile strength ,elongation and notched impact strength can be improved to reach 103%、76.2% and 84.4%, respectively , and the color difference has decreased from 7.6 to 0.8,which is far better than the corresponding properties of POM without light stabilization modification .

参考文献

[1] 任显诚,赵红军,蔡绪福,陈山玉,淡宜.光屏蔽剂对聚甲醛耐老化性能的影响[J].中国塑料,2005(04):78-81.
[2] 赵红军,蔡绪福,陈山玉,任显诚,淡宜.聚甲醛耐老化性能及其改进研究[J].塑料工业,2004(04):19-21.
[3] 王俊,揭敢新.聚甲醛耐候性研究[J].装备环境工程,2006(05):44-47,62.
[4] 吴桂波,赵国栋,王军,任显诚.P(MMA-BA-BPMA)的合成及其改性聚甲醛光稳定性的研究[J].塑料工业,2010(03):36-39.
[5] 杨凡,张适龄,游斌,任显诚.聚丙烯酸酯接枝纳米ZnO弹性体的制备及其对POM稳定性的研究[J].塑料工业,2011(12):26-29.
[6] 于建.聚甲醛的制备、特性及应用[J].工程塑料应用,2001(03):41-44.
[7] N Grassie;R S Roche .The thermal degradation of polyoxymethylene[J].Macromolecular Chemistry and Physics,1968,112(01):16-33.
[8] 李晖,齐晓亮,张广玉,魏莉萍,王湘明,张孝兰.聚甲醛加速老化试验研究[J].工程塑料应用,2002(12):40-43.
[9] 段怡飞 .聚甲醛的热降解和稳定化研究[D].四川大学,2004.
上一张 下一张