Sulfide stress corrosion cracking (SSCC) behaviour of UNS G11180 steel in 5% NaCl solution with H2S was studied by slow strain rate tensile test (SSRT), SEM and electrochemical hydro gen permeation technique. The results reveal different cracking mechanism and H permeation current (IH) through UNS G11180 steel plate in different concentration of H2S solution. The susceptibility to SSCC of UNS G11180 Steel in 5% NaCl solution with H2S was evaluated by the permeation current(IH, μA), which depends on the concentration (c×10-6) of H2S by the equation:IH = 8.525 ×c0.7249. lt is proved that the electrochemical H permeation method is a practical way to assess the susceptibility to SSCC.